When a lining fails early, it is tempting to blame the material. Often the cause is a mix of material, installation and operation.
Material causes
- Moisture picked up during storage.
- Wrong grading for the furnace size, or segregation in the bag.
- Iron or other impurities.
- Binder level too high or too low for the practice.
Installation causes
- Layers too thick or not compacted well.
- Former off-centre, giving a thin side.
- Air pockets left in the wall.
- Foreign material dropped into the mass.
Sintering causes
- Heating too fast at the start, causing cracks.
- Not reaching or holding the full sintering temperature, leaving a thin sintered face.
- Interrupting the first heat.
Operating causes
- Heavy scrap dropped onto the lining.
- Wet or oily charge.
- Long cold periods, then fast reheating.
- Slag chemistry that attacks silica, such as strongly basic slags.
- Overheating the bath well above normal tapping temperature.
How to find the real cause
Look at the old lining when you break it out. Note where it failed, how deep the sintered layer went, and whether metal penetrated cracks. Compare with your lining log. Share photos with your supplier; patterns are often obvious to an experienced eye.